12C27M is a very pure, fine-grained alloy. It has excellent corrosion resistance and is a ‘dishwasher’ safe alloy. It takes incredibly sharp edges and will suit kitchen knives, or skinning knives.
Chemical Composition:-
C:
|
Cr:
|
Mn:
|
Si:
|
P:
|
S:
|
0.52%
|
14.5%
|
0.6%
|
0.4%
|
0.025%
|
0.01%
|
Suggested Heat Treatments:
Heat to 1080C (Hold for 5 minutes)
Air or Oil Quench (Suggested Oil is Rye 32)
Optional – Cool to -70C
Temper twice for two hours at 175C for 58/59HRc or 225C for 56HRc
Supplied Cold Rolled Annealed in 600mm Lengths